Titanium Alloys - Ti11Sn5Zr2.5Al1Mo0.2Si Physical and Mechanical Properties and Fabrication

化学式

ti11sn5zr2.5al1mo0.2si

Background

ti11sn5zr2.5al1mo0.2si, also known as Timetal 679 is a three-phase titanium alloy having an alpha + beta + compound structure at about 950°C (1742°F). To develop optimum mechanical properties, hot working should be restricted to the alpha + beta + compound phase.

Composition

表格1。Ti4al4MO4SN0.5SI0.1C的组成。

内容

Sn

10.5-11.5%

ZR

4.0-6.0%

Al

2.0-2.5%

0.8-1.2%

Si

0.10-0.50%

Fe

<0.20%

H2

<0.0125%

Ti

平衡

Designations

Other designations for Ti11Sn5Zr2.5Al1Mo0.2Si include:

BS TA18 Bar – 50mm ruling section

BS TA19 Forging Stock – 50mm ruling section

BS TA20字子 - 50毫米统治部分

BS TA25 Bar - 75mm ruling section

BS TA26锻造库存-75mm统治部分

BS TA27 Forgings - 75mm ruling section

Key Properties

物理特性

表2。TI11SN5ZR2.5AL1MO0.2SI的典型物理特性。

财产

典型的价值

Density g/cm3(lb/ cu in)

4.84 (0.174)

Mean Co-Eff of Thermal Expansion 20-100°C/°C 68-212°F/°F

8.2x10-6(4.6)

Mean Co-Eff of Thermal Expansion 20-300°C/°C 68-572°F/°F

9.3x10-6(5.2)

Mean Co-Eff of Thermal Expansion 20-500°C/°C 68-932°F/°F

9.6x10-6(5.3)

Beta Transus °C±15°C (°F)

945(1730)

机械性能

Table 3.典型的mechanical properties for Ti11Sn5Zr2.5Al1Mo0.2Si.

财产

典型的

0.2% Proof Stress MPa (ksi)

970 (141)

Tensile Strength MPa (ksi) sheet

1110(161)

Elongation on 1 inch %

8.0

降低面积%

25

Elastic Modulus GPa (Msi)

115 (17)

Fabrication

溶液处理-900°C(1650°F)每25mm截面1小时,AC/OQ

Ageing - 500°C (930°F) 24hr, AC

资料来源:钛信息组

有关此消息来源的更多信息,请访问The Titanium Information Group